Ravenscrag Recipe E: Raspberry Glossy| Code | GR6-E |
| Modification Date | 2011-01-31 15:25:10 |
| Member of Group | RV6 |
| Description | Plainsman Cone 6 Ravenscrag Slip Glaze |
Recipe| Material | Amount | Units | +/- | *Stat |
| Ravenscrag Slip | 70.00 | kg | | |
| Ferro Frit 3134 | 20.00 | kg | | |
| Whiting | 10.00 | kg | | |
| Tin Oxide | 7.50 | kg | | |
| Chrome Oxide | 0.50 | kg | | |
| | 108.00 | |
Firing Schedule
| Rate (C) | Temp (C) | Hold (Min) | Step | | 55 | 104 | 120 | 1 | | 167 | 482 | 0 | 2 | | 83 | 593 | 0 | 3 | | 167 | 945 | 0 | 4 | | 60 | 1185 | 20 | 5 | | 278 | 1035 | 0 | 6 | | 83 | 816 | 0 | 7 |
|