Ravenscrag Recipe C: White Glossy

CodeGR6-C
Modification Date2011-08-03 12:06:43
Member of GroupRV6
DescriptionPlainsman Cone 6 Ravenscrag Slip Glaze

Recipe

MaterialAmountUnits+/-*Stat
Ravenscrag Slip80.00kg  
Ferro Frit 313420.00kg  
Zircopax12.00kg  
 112.00  

Firing Schedule

Rate (C)Temp (C)Hold (Min)Step
551041201
16748202
8359303
16794504
601185205
278103506
8381607