Ravenscrag Recipe B: Variegated Light Glossy Blue| Code | GR6-B |
| Modification Date | 2011-08-03 12:17:09 |
| Member of Group | RV6 |
| Description | Plainsman Cone 6 Ravenscrag Slip Glaze |
Recipe| Material | Amount | Units | +/- | *Stat |
| Ravenscrag Slip | 80.00 | g | | |
| Ferro Frit 3134 | 20.00 | g | | |
| Cobalt Oxide | 3.00 | g | | c |
| Rutile | 3.00 | g | | v |
| Titanium Dioxide | 3.00 | g | | o |
| | 109.00 | |
* c-colorant, v-variegator, o-opacifier, s-suspenderFiring Schedule
| Rate (C) | Temp (C) | Hold (Min) | Step | | 55 | 104 | 120 | 1 | | 167 | 482 | 0 | 2 | | 83 | 593 | 0 | 3 | | 167 | 945 | 0 | 4 | | 60 | 1185 | 20 | 5 | | 278 | 1035 | 0 | 6 | | 83 | 816 | 0 | 7 |
Out Bound Links
In Bound Links
- (Recipes)
G1214W - Cone 6 Transparent Base
- 2003-06-21
- (Recipes - Related)
GR6-A - Ravenscrag Recipe A: Clear Glossy
Plainsman Cone 6 Ravenscrag Slip Glaze
2003-07-21 - -This recipe is a clear even glossy glaze with a s...
Pictures Ravenscrag Recipe B Light blue

Small porcelain vase

|
Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
|
|
INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()
|
|