Ravenscrag Cone 6 Floating Blue

CodeGR6-I
Modification Date2011-08-05 12:20:02
Member of GroupRV6
DescriptionPlainsman Cone 6 Ravenscrag Slip Glaze

Recipe

MaterialAmountUnits+/-*Stat
Ravenscrag Slip70.00kg  
Light Magnesium Carbonate2.00kg  
Dolomite13.00kg  
Ferro Frit 313415.00kg  
Rutile5.00kg  
Cobalt Oxide2.00kg  
Copper Oxide Black1.00kg  
 108.00  

Firing Schedule

Rate (C)Temp (C)Hold (Min)Step
551041201
16748202
8359303
16794504
601185205
278103506
8381607

Notes

David Shaners cone 6 floating blue has been used for many years by thousands of potters. However it contains gerstley borate which is no longer available (see GerstleyBorate.com for information in this classic recipe and the material). In addition it is a temperamental recipe and is prone to blistering. This version is much more reliable and has all the other benefits afforded by a high Ravenscrag content.

Application should be thin to medium and a fast cool down is required to prevent crystallization. It can be fired to cone 5 or 6.


1-79

Out Bound Links

The future of ceramic recipe, material and physical testing record keeping is here.
Watch the video or sign-up at http://insight-live.com.

Maintain your recipe database on-line

  • Login to a private account or work with others in a group account (e.g. university).
  • Nothing to install (access it using your web browser). It is always the latest version.
  • Easy to import your existing data.
  • As many side-by-side recipes as you want.
  • Many ways to search and classify glaze and body recipes.
  • Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
  • Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
  • Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
  • Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
  • Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
  • It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).

Imports many file formats

  • Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
  • Assign a batch number to imports, and later search by batch.
  • Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
  • Prepend character sequences to glaze recipe names during import.
  • Import the pictures and pair them to their corresponding records automatically.
  • One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
  • Export and import individual glaze recipes as text or XML.

Perfect for Education

  • Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
  • Students already have internet connected devices, computers are not even needed in the class.
  • The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()