Cone 06-04 Glossy Base Recipe

CodeG1916M
Modification Date2012-03-27 12:04:40
DescriptionExpansion adjustable frit, kaolin mix

Recipe

MaterialAmountUnits+/-*Stat
Frit 313440.00g  
Frit 312440.00g  
EPK15.00g  
Silica5.00g  
 100.00  

Firing Schedule

Rate (C)Temp (C)Hold (Min)Step
100100601
15096002
100106053
Freefall304

Notes

This is an example of an expansion adjustable transparent base glaze recipe (we have a separate article about this G1916M base). If it crazes, use more Frit 3124 and less Frit 3134; if it shivers use more 3134 and less 3124. If it is too glossy, use Frit 3195 instead of 3124.


1-38

Mechanisms

  • Body Maturity - Mullite Formation

    Assists in the formation of mullite at lower temperatures than formed by conventional alumina-silica sources.

  • Body Plasticity - Extrusion

    Moderately high percentages of the Alkatrol products can be substituted in body compositions to reduce laminations in pressing and to aid in extrusion.

  • Body Thermal Expansion -

    Add this to reduce thermal expansion and reduce firing shrinkage.

Out Bound Links

In Bound Links

The future of ceramic recipe, material and physical testing record keeping is here.
Watch the video or sign-up at http://insight-live.com.

Maintain your recipe database on-line

  • Login to a private account or work with others in a group account (e.g. university).
  • Nothing to install (access it using your web browser). It is always the latest version.
  • Easy to import your existing data.
  • As many side-by-side recipes as you want.
  • Many ways to search and classify glaze and body recipes.
  • Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
  • Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
  • Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
  • Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
  • Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
  • It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).

Imports many file formats

  • Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
  • Assign a batch number to imports, and later search by batch.
  • Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
  • Prepend character sequences to glaze recipe names during import.
  • Import the pictures and pair them to their corresponding records automatically.
  • One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
  • Export and import individual glaze recipes as text or XML.

Perfect for Education

  • Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
  • Students already have internet connected devices, computers are not even needed in the class.
  • The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()