Alberta Slip Deep Brown Cone 6| Code | G2415G |
| Modification Date | 2011-07-20 10:19:13 |
| Member of Group | ASlip |
Recipe| Material | Amount | Units | +/- | *Stat |
| Ferro Frit 3195 | 21.00 | g | | |
| Lithium Carbonate | 5.00 | g | | |
| Alberta Slip | 75.00 | g | | |
| Calcined Alumina | 5.00 | g | | |
| Tin Oxide | 4.00 | g | | |
| | 110.00 | |
Firing Schedule
| Rate (C) | Temp (C) | Hold (Min) | Step | | 55 | 104 | 120 | 1 | | 167 | 482 | 0 | 2 | | 83 | 593 | 0 | 3 | | 167 | 945 | 0 | 4 | | 60 | 1185 | 20 | 5 | | 278 | 1035 | 0 | 6 | | 83 | 816 | 0 | 7 |
Out Bound Links
In Bound Links
- (Recipes - Related)
GA6-A - Alberta Slip Cone 6 Base Glaze
2003-12-12 - Covers very well to produce a transparent amber gl... - (Recipes - Related)
G2863 - Alberta Slip Black Cone 6
2003-12-12 - A glossy black. Should be ball milled.
Pictures This is the class 11 Lithium, 4 Tin, 85 Alberta slip glaze with 5% added alumina calcined

Chocolate brown glossy Alberta Slip glaze uses 5% lithium, 4% tin, 20% frit 3195 with 5% alumina

This 1 inch tal mugs was made using Alberta slip plus some lithium, tin, frit and calcined alumina.

|