WRA Calcined Alumina
ALUMINA
This is an intermediate soda, medium crystalline 3rd generation calcined
alumina.
WRA A-17 A-16
Ultimate crystal size d50-Eppendorf, microns: 2.5-3.2 3.0-3.5 .3-.5
Al2O3 99.5+ 99.5+
SiO2 .02 for A17, .01 for A16
Fe2O3 .01 for all
Na2O3 .08 for A17 and A16
Specific surface area: BET, m2/g .5-.8 3 3-7
Aggregate size, % for WRA: >150 micron 1-10, >63 " 60-80, >40 70-95
Grinding time, Hrs: 4 for A17, 16 for A16
Green density, g/cc: 2.15 for A16, 2.5 for A17
Fired density, g/cc: 3.88 for A16, 3.75 for A17
From Aluminum Company of America
1501 Alcoa Building
Chemicals Division
Pittsburg, PA 15219
Out Bound Links
XML for Import into INSIGHT
<?xml version="1.0" encoding="UTF-8"?>
<material name="WRA Calcined Alumina" descrip="ALUMINA" searchkey="" loi="0.10" casnumber="">
<oxides>
<oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.020" tolerance=""/>
<oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.100" tolerance=""/>
<oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="99.700" tolerance=""/>
<oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="0.020" tolerance=""/>
<oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.020" tolerance=""/>
</oxides>
<volatiles>
<volatile symbol="LOI" name="Loss on Ignition" percent="0.100" tolerance=""/>
</volatiles>
</material> |
The future of ceramic recipe, material and physical testing record keeping is here.
Maintain your recipe database on-line
- Login to a private account or work with others in a group account (e.g. university).
- Nothing to install (access it using your web browser). It is always the latest version.
- Easy to import your existing data.
- As many side-by-side recipes as you want.
- Many ways to search and classify glaze and body recipes.
- Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
- Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
- Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
- Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
- Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
- It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).
Imports many file formats
- Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
- Assign a batch number to imports, and later search by batch.
- Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
- Prepend character sequences to glaze recipe names during import.
- Import the pictures and pair them to their corresponding records automatically.
- One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
- Export and import individual glaze recipes as text or XML.
Perfect for Education
- Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
- Students already have internet connected devices, computers are not even needed in the class.
- The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..
|