Standard Porcelain Kaolin
A white burning high strength Cornish kaolin
| PCE - Pyrometric Cone Equivalent |
33 |
A popular kaolin from the UK.
Particle Size Distribution:
>53 microns: 0.03 max
>10 microns: 4
<2 microns: 70
Modulus of Rupture, Kgf/cm2:
At 80% Relative Humidity: 14.0
Dried at 110C: 31.7
Casting Rate @ 63% solids (mm2/min): 0.35
% P84 Deflocculant Required for 5 Poise Slip: 0.75
1180C 1280C 1410C
Fired Absorption: 15% 6% 1%
Fired Shrinkage: 9% 14% 17%
Brightness: 91 88 77
Out Bound Links
- (Minerals - Contains)
Mica
See Muscovite.
- (Minerals - Contains)
Kaolinite
The most fundamental clay mineral. It is weathered... - (Materials - Related)
Grolleg Kaolin - Fine White Burning English Kaolin, English China Clay
Grolleg China Clay
- (Materials - Related)
Super Standard Porcelain - White burning high strength Cornish kaolin
Super Standard Porcelain Kaolin
- (Materials - Parent)
English Kaolin - Al2O3.SiO2 - White Burning High Flux Kaolin
- (Materials - Parent)
Kaolin - Al2O3.2SiO2 or Al2Si2O5(OH)4 - Hydrated alumina silicate, Pure clay mineral
China Clay
- (MDT - Member)
UK
We are working on this database and would apprecia... - (Typecodes - Type)
1: KAO - Kaolin
- (MDT - Member)
North America
The decision about what materials to include in th... - (MDT - Member)
Europe
Countries of Eastern Europe and former Soviet Unio... - (MDT - Member)
Asia
All of Asia including Turkey, Russia, Indosnesia, ... - (MDT - Member)
Australia
We are working on this database and would apprecia... - (MDT - Member)
Latin and South America
Latin America and South America. We are working on... - (MDT - Member)
Africa
All of continental Africa. We are working on this ... - (MDT - Member)
Ron Roy
This is the traditional Ron Roy materials file. He... - (MDT - Member)
New Zealand
We are working on this database and would apprecia...
In Bound Links
XML for Import into INSIGHT
<?xml version="1.0" encoding="UTF-8"?>
<material name="Standard Porcelain Kaolin" descrip="A white burning high strength Cornish kaolin" searchkey="English Standard Porcelain, Eng Stn Porc, Standard Porcelain China Clay" loi="0.00" casnumber="95077-05-7">
<oxides>
<oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.100" tolerance=""/>
<oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.300" tolerance=""/>
<oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.600" tolerance=""/>
<oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.100" tolerance=""/>
<oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.030" tolerance=""/>
<oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="37.000" tolerance=""/>
<oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="48.000" tolerance=""/>
<oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.600" tolerance=""/>
</oxides>
<volatiles>
<volatile symbol="LOI" name="Loss on Ignition" percent="12.400" tolerance=""/>
</volatiles>
</material> |
The future of ceramic recipe, material and physical testing record keeping is here.
Maintain your recipe database on-line
- Login to a private account or work with others in a group account (e.g. university).
- Nothing to install (access it using your web browser). It is always the latest version.
- Easy to import your existing data.
- As many side-by-side recipes as you want.
- Many ways to search and classify glaze and body recipes.
- Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
- Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
- Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
- Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
- Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
- It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).
Imports many file formats
- Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
- Assign a batch number to imports, and later search by batch.
- Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
- Prepend character sequences to glaze recipe names during import.
- Import the pictures and pair them to their corresponding records automatically.
- One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
- Export and import individual glaze recipes as text or XML.
Perfect for Education
- Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
- Students already have internet connected devices, computers are not even needed in the class.
- The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..
|