Spinks Special Clay

Chemistry %

CaO0.22
MgO0.27
K2O0.28
Na2O0.14
P2O50.11
TiO21.52
Al2O327.17
SiO259.16
Fe2O31.15
MnO0.02
 

Volatiles %

LOI10.16
SO30.02

Relative Viscosity (1.2 Sp. Gr.):* 1.27
Casting Rate: (gms per 15 min/426 cm2):* 158
Water of Plasticity:* 17.07
% Dry Shrinkage:* 4.9
Dry M.O.R., psi:* 593

Cone 04 8 11
----
Fired Shrinkage:* 0.1% 1.3% 1.2%
Absorption:* 15.9% 13.6% 13.4%
M.O.R. psi:* 1427 3901 3970

Thermal Expansion, Cone 8: .397% at 700C
P.C.E.: 32
pH: 4.8
Oil Absorption: 35
Bulk Density, lbs per cubic foot: 34-39
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
96% 92% 82% 64% 47% 29% 7%

*Specimens: De-aired, extruded, 50% ball clay, 50% flint


Out Bound Links

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Spinks Special Clay" descrip="" searchkey="" loi="10.18" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.220" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.270" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.280" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.140" tolerance=""/> <oxide symbol="P2O5" name="Phosphorus Pentoxide" status="" percent="0.110" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.520" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="27.170" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="59.160" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.150" tolerance=""/> <oxide symbol="MnO" name="Manganous Oxide" status="" percent="0.020" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="10.160" tolerance=""/> <volatile symbol="SO3" name="Sulfur Trioxide" percent="0.020" tolerance=""/> </volatiles> </material>
The future of ceramic recipe, material and physical testing record keeping is here.
Watch the video or sign-up at http://insight-live.com.

Maintain your recipe database on-line

  • Login to a private account or work with others in a group account (e.g. university).
  • Nothing to install (access it using your web browser). It is always the latest version.
  • Easy to import your existing data.
  • As many side-by-side recipes as you want.
  • Many ways to search and classify glaze and body recipes.
  • Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
  • Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
  • Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
  • Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
  • Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
  • It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).

Imports many file formats

  • Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
  • Assign a batch number to imports, and later search by batch.
  • Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
  • Prepend character sequences to glaze recipe names during import.
  • Import the pictures and pair them to their corresponding records automatically.
  • One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
  • Export and import individual glaze recipes as text or XML.

Perfect for Education

  • Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
  • Students already have internet connected devices, computers are not even needed in the class.
  • The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()