Palestone

Plainsman Native Clay

Chemistry %

BaO0.32
CaO0.22
MgO0.56
K2O2.32
Na2O0.14
P2O50.15
TiO20.65
Al2O317.20
SiO270.43
Fe2O31.30
MnO0.01
 

Volatiles %

LOI6.70
MLPT - Melting Point (MP) PCE 22

A pale firing stoneware with good plasticity and suitable for making up the major part of a mix. It develops maturity in the cone 8-11 range and is fine grained and strong. This is material is balanced enough to use by itself.

Fired Temperature, Cone 6 7 8 9 10 11 10R
--------------------------------------------
Fired Shrinkage: 4.4% 4.6% 4.8% 5.1% 5.4% n/a n/a
Absorption: 3.8% 3.2% 2.6% 2.0% 1.0% n/a n/a
Fired Strength:
(lbs/ square inch) 5800 6200 6700 7100 7100

Sieve Analysis Wet Washed
(Root of 2 series) +35 +48 +65 +100 +150# +200 +325
--------------------------------------------
0.1% 0.3% 1.9% 6.3% 9.1% 13.6% 21.5%

Texture: Sl. tooth
Plastic Index (1-10): 6
Green Strength (lbs/sqaure inch): 950
Dry shrinkage: 6.0
Dried density: 2.04
PCE: 21.5


Out Bound Links

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Palestone" descrip="Plainsman Native Clay" searchkey="" loi="6.70" casnumber="70694-09-6"> <oxides> <oxide symbol="BaO" name="Barium Oxide, Baria" status="" percent="0.320" tolerance=""/> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.220" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.560" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="2.320" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.140" tolerance=""/> <oxide symbol="P2O5" name="Phosphorus Pentoxide" status="" percent="0.150" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.650" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="17.200" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="70.430" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.300" tolerance=""/> <oxide symbol="MnO" name="Manganous Oxide" status="" percent="0.010" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="6.700" tolerance=""/> </volatiles> </material>
The future of ceramic recipe, material and physical testing record keeping is here.
Watch the video or sign-up at http://insight-live.com.

Maintain your recipe database on-line

  • Login to a private account or work with others in a group account (e.g. university).
  • Nothing to install (access it using your web browser). It is always the latest version.
  • Easy to import your existing data.
  • As many side-by-side recipes as you want.
  • Many ways to search and classify glaze and body recipes.
  • Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
  • Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
  • Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
  • Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
  • Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
  • It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).

Imports many file formats

  • Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
  • Assign a batch number to imports, and later search by batch.
  • Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
  • Prepend character sequences to glaze recipe names during import.
  • Import the pictures and pair them to their corresponding records automatically.
  • One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
  • Export and import individual glaze recipes as text or XML.

Perfect for Education

  • Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
  • Students already have internet connected devices, computers are not even needed in the class.
  • The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()