Chemistry %

CaO0.23
MgO0.01
K2O12.04
Na2O1.45
Al2O317.94
B2O30.92
SiO264.46
Fe2O30.04
 

Volatiles %

LOI0.70
SAMG - Surface Area (m2/gm) 1.4
BDLB - Bulk Density lbs/cu. ft. (Packed) 40 loose, 60 packed
AVPS - Average Particle Size (Microns) 8.0

The company was introducing this material during late 2006 and calls it "a high quality potassium/sodium/calcium aluminum silicate ground to 325 mesh for ceramic applications." "It offers a high potash and low iron oxide content per unit of alumina and is particularly suited for use in glazes".
Cone 11 fired flow tests beside MC Na-200 show that this does not melt nearly as well.
The melt flow is whiter than G-200 and much whiter than Custer.


Out Bound Links

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="MC K-325 Feldspar" descrip="" searchkey="MC K325, K325" loi="0.00" casnumber="12168-80-8"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.230" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.010" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="12.040" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="1.450" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="17.940" tolerance=""/> <oxide symbol="B2O3" name="Boric Oxide" status="" percent="0.920" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="64.460" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.040" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="0.700" tolerance=""/> </volatiles> </material>
The future of ceramic recipe, material and physical testing record keeping is here.
Watch the video or sign-up at http://insight-live.com.

Maintain your recipe database on-line

  • Login to a private account or work with others in a group account (e.g. university).
  • Nothing to install (access it using your web browser). It is always the latest version.
  • Easy to import your existing data.
  • As many side-by-side recipes as you want.
  • Many ways to search and classify glaze and body recipes.
  • Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
  • Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
  • Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
  • Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
  • Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
  • It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).

Imports many file formats

  • Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
  • Assign a batch number to imports, and later search by batch.
  • Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
  • Prepend character sequences to glaze recipe names during import.
  • Import the pictures and pair them to their corresponding records automatically.
  • One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
  • Export and import individual glaze recipes as text or XML.

Perfect for Education

  • Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
  • Students already have internet connected devices, computers are not even needed in the class.
  • The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()