KTS-Classic
Tennessee Ball Clay
A combination of Kentucky and Tennessee Ball Clays with very good overall plasticity and strength. KTS-Classic can be used in casting or plastic formed bodies. It is also supplied in a clay-water slurry form for use by the sanitaryware and artware industries.
Physical Properties
===================
Water of Plasticity*: 37.0%
% Dry Shrinkage*: 6.5
Dry M.O.R., psi:* 825
pH: 4.4
C.E.C., meq/100g: 11.0
Specific Surface Area, sq metre/g: 24.4
Soluble sulfur+: Low
P.C.E.: 32
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
(% finer than) 99% 97% 93% 81% 72% 56% 35%
Fired Properties
================
Cone 5 10
----
Total Shrinkage: 13.0% 14.5%
Absorption: 10.0% 1.0%
Shipped from Mayfield, KY
------------------
*Extruded, 50% ball clay, 50% flint
+Low-trace to 150, Med-150-400, High-450+
**50% Clay, 50% Nepheline Syenite
Out Bound Links
XML for Import into INSIGHT
<?xml version="1.0" encoding="UTF-8"?>
<material name="KTS-Classic" descrip="Tennessee Ball Clay" searchkey="" loi="0.00" casnumber="70694-09-6">
<oxides>
<oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.300" tolerance=""/>
<oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.500" tolerance=""/>
<oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.400" tolerance=""/>
<oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.200" tolerance=""/>
<oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.400" tolerance=""/>
<oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="24.600" tolerance=""/>
<oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="61.100" tolerance=""/>
<oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.000" tolerance=""/>
</oxides>
<volatiles>
<volatile symbol="LOI" name="Loss on Ignition" percent="9.500" tolerance=""/>
</volatiles>
</material> |
The future of ceramic recipe, material and physical testing record keeping is here.
Maintain your recipe database on-line
- Login to a private account or work with others in a group account (e.g. university).
- Nothing to install (access it using your web browser). It is always the latest version.
- Easy to import your existing data.
- As many side-by-side recipes as you want.
- Many ways to search and classify glaze and body recipes.
- Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
- Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
- Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
- Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
- Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
- It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).
Imports many file formats
- Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
- Assign a batch number to imports, and later search by batch.
- Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
- Prepend character sequences to glaze recipe names during import.
- Import the pictures and pair them to their corresponding records automatically.
- One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
- Export and import individual glaze recipes as text or XML.
Perfect for Education
- Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
- Students already have internet connected devices, computers are not even needed in the class.
- The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..
|