Digitalfire Ceramic Materials Database

Logged in as Level 2 access: Logout


HC#5 Clay

Ball Clay

Chemistry %

CaO0.27
MgO0.21
K2O0.31
Na2O0.10
P2O50.14
TiO21.59
Al2O327.65
SiO256.25
Fe2O31.13
MnO0.02
 

Volatiles %

LOI12.40
SO30.03

Particle Size Distribution:
>53 microns: 0.10 max
>10 microns: 18
<2 microns: 44

Modulus of Rupture, Kgf/cm2:
At 80% Relative Humidity: 7.5
Dried at 110C: 16.2

Casting Rate @ 62% solids (mm2/min): 2.0
% P84 Deflocculant Required for 5 Poise Slip: 0.6

1180C 1280C
Fired Absorption: 15% 6%
Fired Shrinkage: 9% 13%
Brightness: 84 84


Out Bound Links

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="HC#5 Clay" descrip="Ball Clay" searchkey="" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.270" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.210" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.310" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.100" tolerance=""/> <oxide symbol="P2O5" name="Phosphorus Pentoxide" status="" percent="0.140" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.590" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="27.650" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="56.250" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.130" tolerance=""/> <oxide symbol="MnO" name="Manganous Oxide" status="" percent="0.020" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="12.400" tolerance=""/> <volatile symbol="SO3" name="Sulfur Trioxide" percent="0.030" tolerance=""/> </volatiles> </material>
The future of ceramic recipe, material and physical testing record keeping is here.
Watch the video or sign-up at http://insight-live.com.

Maintain your recipe database on-line

  • Login to a private account or work with others in a group account (e.g. university).
  • Nothing to install (access it using your web browser). It is always the latest version.
  • Easy to import your existing data.
  • As many side-by-side recipes as you want.
  • Many ways to search and classify glaze and body recipes.
  • Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
  • Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
  • Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
  • Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
  • Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
  • It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).

Imports many file formats

  • Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
  • Assign a batch number to imports, and later search by batch.
  • Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
  • Prepend character sequences to glaze recipe names during import.
  • Import the pictures and pair them to their corresponding records automatically.
  • One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
  • Export and import individual glaze recipes as text or XML.

Perfect for Education

  • Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
  • Students already have internet connected devices, computers are not even needed in the class.
  • The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()