F. C. Kaolin
COARSE GRAINED GEORGIA KAOLIN
Originally referred to as FAST CAST, F.C. Clay is a secondary, coarse grained Georgia Clay with a particle size distribution approaching that of fractional clay. The chemical analysis is close to that of theoretical kaolinite. Uniformity, excellent color, low C.E.C., surface area, ease of dispersion and coarseness are notable characteristics. It is available in lump, dried, airfloated and slurry forms.
PCE: 34
+325 Residue (%): 1
pH: 4.5-6.5
C.E.C.: 2.00
Specific Gravity: 2.62
Casting Rate gms/30'(Bariod): 120
Bulk Density: 30#/c. ft.
% finer than 10 microns: 96
10 microns: 87
5 microns: 71
2 microns: 49
1 micron: 37
0.5 micron: 24
Median particle diameter (microns): 2.0
Specific surface area (sq. meters/gram): 10.0
Out Bound Links
- (Materials - Parent)
Kaolin - Al2O3.2SiO2 or Al2Si2O5(OH)4 - Hydrated alumina silicate, Pure clay mineral
China Clay
- (Typecodes - Type)
1: KAO - Kaolin
XML for Import into INSIGHT
<?xml version="1.0" encoding="UTF-8"?>
<material name="F. C. Kaolin" descrip="COARSE GRAINED GEORGIA KAOLIN" searchkey="" loi="13.51" casnumber="95077-05-7">
<oxides>
<oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.040" tolerance=""/>
<oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.020" tolerance=""/>
<oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.110" tolerance=""/>
<oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.020" tolerance=""/>
<oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.770" tolerance=""/>
<oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="38.210" tolerance=""/>
<oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="45.160" tolerance=""/>
<oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.360" tolerance=""/>
</oxides>
<volatiles>
<volatile symbol="LOI" name="Loss on Ignition" percent="13.510" tolerance=""/>
</volatiles>
</material> |
The future of ceramic recipe, material and physical testing record keeping is here.
Maintain your recipe database on-line
- Login to a private account or work with others in a group account (e.g. university).
- Nothing to install (access it using your web browser). It is always the latest version.
- Easy to import your existing data.
- As many side-by-side recipes as you want.
- Many ways to search and classify glaze and body recipes.
- Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
- Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
- Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
- Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
- Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
- It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).
Imports many file formats
- Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
- Assign a batch number to imports, and later search by batch.
- Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
- Prepend character sequences to glaze recipe names during import.
- Import the pictures and pair them to their corresponding records automatically.
- One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
- Export and import individual glaze recipes as text or XML.
Perfect for Education
- Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
- Students already have internet connected devices, computers are not even needed in the class.
- The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..
|