F-4 Feldspar

Sodium Feldspar

Chemistry %

CaO1.70
MgO0.05
K2O4.80
Na2O6.90
Al2O319.60
SiO266.80
Fe2O30.04
 

Volatiles %

LOI0.20

Shipped from Spruce Pine, North Carolina. No longer available. Minspar 200 (formerly NC4) has virtually identical chemistry to F-4 and should be a good substitute.

Particle sizes:
+100 mesh: trace
+140: .1
+170: .1
+200: .2
+325: 3.8

This material is prized as a porcelain ingredient because of its low iron content. It is used in casting and throwing porcelains of all types. At cone 6 for example, it is possible to make a vitreous body using 50-60%. However to get enough plasticity in such bodies, it is necessary to use ball clay or bentonite which can darken the color. If high plasticity is not essential, Macaloid and plastic kaolins can be used.

Another similar material is Nepheline Syenite.


Out Bound Links

  • (Materials - Alternative) C-6 Feldspar - SODA FELDSPAR
  • (Materials - Related) Nepheline Syenite - Generic

    Neph Sy

  • (Materials - Substitute) Minspar 200 - Feldspar
  • (Typecodes - Type) 1: FEL - Feldspar
  • (MDT - Member) North America

    The decision about what materials to include in th...

  • (MDT - Member) Europe

    Countries of Eastern Europe and former Soviet Unio...

  • (MDT - Member) Asia

    All of Asia including Turkey, Russia, Indosnesia, ...

  • (MDT - Member) Australia

    We are working on this database and would apprecia...

  • (MDT - Member) Latin and South America

    Latin America and South America. We are working on...

  • (MDT - Member) Africa

    All of continental Africa. We are working on this ...

  • (MDT - Member) Ron Roy

    This is the traditional Ron Roy materials file. He...

  • (MDT - Member) Crystal Glazes

    These materials are specially defined for makers o...

  • (MDT - Member) New Zealand

    We are working on this database and would apprecia...

  • (Materials - Substitute) NC-4 Feldspar

    NC4 Feldspar, Spruce Pine #4 Spar

In Bound Links

  • (Materials - Related) Unispar 50 - Soda Feldspar

    Unispar-50

  • (Materials - Related) G-200 Feldspar - Potash/sodium/calcium 200 mesh Feldspar

    G200 Feldspar, G200 Spar, G 200 Spar, G 200, G 200 Feldspar

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="F-4 Feldspar" descrip="Sodium Feldspar" searchkey="F4 Feldspar, Kona Feldspar, Kona F4, F4 Spar, F 4 Feldspar" loi="0.00" casnumber="12168-80-8"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="U" percent="1.700" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="U" percent="0.050" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="U" percent="4.800" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="U" percent="6.900" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="19.600" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="66.800" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.040" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="0.200" tolerance=""/> </volatiles> </material>
The future of ceramic recipe, material and physical testing record keeping is here.
Watch the video or sign-up at http://insight-live.com.

Maintain your recipe database on-line

  • Login to a private account or work with others in a group account (e.g. university).
  • Nothing to install (access it using your web browser). It is always the latest version.
  • Easy to import your existing data.
  • As many side-by-side recipes as you want.
  • Many ways to search and classify glaze and body recipes.
  • Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
  • Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
  • Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
  • Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
  • Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
  • It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).

Imports many file formats

  • Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
  • Assign a batch number to imports, and later search by batch.
  • Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
  • Prepend character sequences to glaze recipe names during import.
  • Import the pictures and pair them to their corresponding records automatically.
  • One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
  • Export and import individual glaze recipes as text or XML.

Perfect for Education

  • Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
  • Students already have internet connected devices, computers are not even needed in the class.
  • The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()