Chemistry %

CaO0.30
MgO0.40
K2O1.20
Na2O0.10
TiO21.20
Al2O326.20
SiO255.90
Fe2O31.20
 

Volatiles %

LOI12.50
PCE - Pyrometric Cone Equivalent 32

A fine-grained ball clay used primarily in plastic formed bodies. The colloidal organic present in Dresden M helps contribute excellent strength and plasticity.

Physical Properties
===================
Water of Plasticity*: 37.0%
% Dry Shrinkage*: 6.5
Dry M.O.R., psi:* 825
pH: 4.4
C.E.C., meq/100g: 11.0
Specific Surface Area, sq metre/g: 24.4
Soluble Sulfur: Low

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
(% finer than) 99% 97% 93% 81% 72% 56% 35%

Fired Properties
================
Cone 5 10
----
Total Shrinkage: 13.0% 14.5%
Absorption: 10.0% 1.0%

------------------
*Extruded, 50% ball clay, 50% flint
+Low-trace to 150, Med-150-400, High-450+
**50% Clay, 50% Nepheline Syenite


Out Bound Links

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Dresden M Ball Clay" descrip="Kentucky Ball Clay" searchkey="Dresden Ball Caly" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.300" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.400" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.200" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.100" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.200" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="26.200" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="55.900" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.200" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="12.500" tolerance=""/> </volatiles> </material>
The future of ceramic recipe, material and physical testing record keeping is here.
Watch the video or sign-up at http://insight-live.com.

Maintain your recipe database on-line

  • Login to a private account or work with others in a group account (e.g. university).
  • Nothing to install (access it using your web browser). It is always the latest version.
  • Easy to import your existing data.
  • As many side-by-side recipes as you want.
  • Many ways to search and classify glaze and body recipes.
  • Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
  • Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
  • Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
  • Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
  • Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
  • It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).

Imports many file formats

  • Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
  • Assign a batch number to imports, and later search by batch.
  • Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
  • Prepend character sequences to glaze recipe names during import.
  • Import the pictures and pair them to their corresponding records automatically.
  • One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
  • Export and import individual glaze recipes as text or XML.

Perfect for Education

  • Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
  • Students already have internet connected devices, computers are not even needed in the class.
  • The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()