Ceraclay WTC Kaolin

Chemistry %

CaO0.05
MgO0.30
K2O2.20
Na2O0.10
TiO20.05
Al2O336.50
SiO248.50
Fe2O30.85
 

Volatiles %

LOI11.20

Particle Size Distribution:
>53 microns: 1.0 max
>10 microns: 18
<2 microns: 26

Modulus of Rupture, Kgf/cm2:
At 80% Relative Humidity: 3.0
Dried at 110C: 6.0

Casting Rate @ 65% solids (mm2/min): 6.5
% P84 Deflocculant Required for 5 Poise Slip: 0.40

1180C 1280C
Fired Absorption: 19% 11%
Fired Shrinkage: 6% 10%
Brightness: 84 86


Out Bound Links

  • (Materials - Parent) Kaolin - Al2O3.2SiO2 or Al2Si2O5(OH)4 - Hydrated alumina silicate, Pure clay mineral

    China Clay

  • (Typecodes - Type) 1: KAO - Kaolin

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Ceraclay WTC Kaolin" descrip="" searchkey="" loi="0.00" casnumber="95077-05-7"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.050" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.300" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="2.200" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.100" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.050" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="36.500" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="48.500" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.850" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="11.200" tolerance=""/> </volatiles> </material>
The future of ceramic recipe, material and physical testing record keeping is here.
Watch the video or sign-up at http://insight-live.com.

Maintain your recipe database on-line

  • Login to a private account or work with others in a group account (e.g. university).
  • Nothing to install (access it using your web browser). It is always the latest version.
  • Easy to import your existing data.
  • As many side-by-side recipes as you want.
  • Many ways to search and classify glaze and body recipes.
  • Glaze and body recipes are robust, with units-of-measure, unlimited pictures with individual titles and descriptions.
  • Add variations to a recipe; each with its own pictures, descriptions and name/code-number extensions.
  • Recipes can link to typecodes, projects and firing schedules (all managed in their own areas).
  • Standard reports and mix ticket reports with last-minute-totalling; variations report as if they are a complete recipe.
  • Video tutorials, help system, contact form on every page, dedicated messaging and support ticket systems.
  • It is an industrial-strength database system (unlimited capacity, fast, reliable, scalable).

Imports many file formats

  • Glaze recipe formats supported: HyperGlaze, GlazeGhem, GlazeMaster, Matrix, INSIGHT XML recipes (single and multiple), INSIGHT SQLite DB files.
  • Assign a batch number to imports, and later search by batch.
  • Assign multiple typecodes to imported glaze and body batches (to classify) and search on these later.
  • Prepend character sequences to glaze recipe names during import.
  • Import the pictures and pair them to their corresponding records automatically.
  • One click to automatically export the database to an SQLite DB database file and download it (for use with desktop INSIGHT or just as a backup).
  • Export and import individual glaze recipes as text or XML.

Perfect for Education

  • Ceramic study programs can now accumulate material, recipe and testing data year-after-year, students can login and together build a valuable ceramic glaze and body knowledge resource.
  • Students already have internet connected devices, computers are not even needed in the class.
  • The Reference Manager gives you quick access to the Digitalfire Ceramic Reference Database.
Learn more..



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()